性能項目 | 試驗條件[狀態(tài)] | 測試方法 | 測試數(shù)據(jù) | 數(shù)據(jù)單位 | |
物理性能 | 熔點 | MCI方法 | 240 | ℃ | |
密度 | ASTM D-1505 | 0.833 | g/cm3 | ||
熔融指數(shù) | 260℃,5kg | ASTM D-1238 | 26 | g/10min | |
機械性能 | 抗張強度 | ASTM D-638 | 175 | kg/cm2 | |
Rockwell硬度 | ASTM D-785 | R85 | |||
曲折模數(shù) | ASTM D-790 | 13,000 | kg/cm2 | ||
斷裂伸長率 | ASTM D-638 | 25 | % | ||
曲折強度 | ASTM D-790 | 360 | kg/cm2 | ||
凹口Charpy耐沖擊強度 | ASTM D-256 | 5 | kgcm/cm2 | ||
無凹口lzod耐沖擊強度 | ASTM D-256 | 15 | kgcm/cm2 | ||
Olsen剛性 | ASTM D-747 | 10,000 | kg/cm2 | ||
抗張屈服強度 | ASTM D-638 | 235 | kg/cm2 | ||
電氣性能 | 體積電阻系數(shù) | ASTM D-257 | >1016 | Ωcm | |
吸水率 | 24hr | ASTM D-570 | 0.01 | % | |
介電強度 | ASTM D-149 | 65 | KV/mm | ||
介電常數(shù) | 100~1MHz | ASTM D-150 | 2.12 | ||
介電消散因子 | 23℃,1MHz | ASTM D-150 | 0.0007 | ||
熱性能 | 熱傳導(dǎo)系數(shù) | ASTM BS-847A | 4*10-4 | calcm/seccm2℃ | |
熱變形溫度 | 4.6kg/cm2 | ASTM D-648 | 90 | ℃ | |
線膨脹系數(shù) | ASTM D-696 | 1.17*10-4 | 1/℃ | ||
燃燒速率 | ASTM D-635 | 2.54 | cm/min | ||
模收縮率(機械/垂直方向) | MCI方法 | 2.1/1.7 | % | ||
Vicat軟化點 | ASTM D-1525 | 173 | ℃ | ||
比熱 | ASTM C-351 | 0.47 | cal/g℃ | ||
其它性能 | 折射率 | ASTM D-542 | 1.463 | nd | |
模糊度 | ASTM D-1746 | 1.5 | % | ||
透光率 | ASTM D-1746 | 92 | % |