性能項(xiàng)目 | 試驗(yàn)條件[狀態(tài)] | 測(cè)試方法 | 測(cè)試數(shù)據(jù) | 數(shù)據(jù)單位 | |
物理性能 | 比重 | ASTM D792, ISO 1183 | 1.19 |
g/cm3;
|
|
收縮率 | 流動(dòng): 24小時(shí) | ASTM D955 | 1.0--3.0 | % | |
橫向流動(dòng): 24小時(shí) | ASTM D955 | 1.0-3.0 | % | ||
機(jī)械性能 | 拉伸模量2 | |
ASTM D638 | 3730 | MPa |
抗張強(qiáng)度3 | 斷裂 | ASTM D638 | 52.7 | MPa | |
伸長率3 |
斷裂
|
ASTM D638 | 25 | % | |
彎曲模量4 |
|
ASTM D790 | 2150 | MPa | |
彎曲強(qiáng)度 | ASTM D790 | 78.0 | MPa | ||
摩擦系數(shù) |
與自身 - 動(dòng)態(tài)
|
ASTM D3702 Modified | 0.60 | ||
與自身 - 靜態(tài)
|
ASTM D3702 Modified | 0.42 | |||
磨損因數(shù) |
Ring
|
ASTM D3702 Modified | 0.300 |
10^-10 in^5-min/ft-lb-hr
|
|
Washer
|
ASTM D3702 Modified | 74.0 |
10^-10 in^5-min/ft-lb-hr
|
||
懸壁梁缺口沖擊強(qiáng)度 | 23°C | ASTM D256 | 48 | J/m | |
23°C 5 |
ISO 180/1A | 4.9 | kJ/m2; | ||
無缺口懸臂梁沖擊 | 23°C |
ASTM D4812 | 1200 | J/m | |
23°C 5 | ISO 180/1U | 68 | kJ/m2; | ||
裝有測(cè)量儀表的落鏢沖擊 | 23°C, Energy at Peak Load | ASTM D3763 | 9.60 | J | |
-- | ISO 6603-2 | 24.7 | J | ||
熱性能 | 熱變形溫度 |
0.45 MPa, 未退火, 3.20 mm
|
ASTM D648 | 144 | °C |
0.45 MPa, 未退火, 64.0 mm 跨距 6
|
ISO 75-2/Bf | 133 | °C | ||
1.8 MPa, 未退火, 3.20 mm
|
ASTM D648 | 54.0 | °C | ||
1.8 MPa, 未退火, 64.0 mm 跨距 6
|
ISO 75-2/Af | 51.0 | °C | ||
線形膨脹系數(shù) |
流動(dòng): -30 到 30°C
|
ASTM D696 | 0.000096 | cm/cm/°C | |
橫向: -30 到 30°C
|
ASTM D696 | 0.000095 | cm/cm/°C |