斷裂伸長率 | 700% | 拉伸強度 | 12MPa | 密度 | 0.921g/cm3 |
熔體流動速率 | 2g/10min | 用途級別 | 薄膜級,纖維 | 規(guī)格級別 | 薄膜 |
缺口沖擊強度 | 130 | 加工級別 | 注塑級 | 特性級別 | 增強級 |
|
產(chǎn)品簡述
斷裂伸長率 | 700% | 拉伸強度 | 12MPa | 密度 | 0.921g/cm3 |
熔體流動速率 | 2g/10min | 用途級別 | 薄膜級,纖維 | 規(guī)格級別 | 薄膜 |
缺口沖擊強度 | 130 | 加工級別 | 注塑級 | 特性級別 | 增強級 |
詳細(xì)數(shù)據(jù)
訂購指南
性能項目 | 試驗條件[狀態(tài)] | 測試方法 | 測試數(shù)據(jù) | 數(shù)據(jù)單位 | ||
基本性能 | 熔體流動速率 | ASTM D-1238 | 2.0 | g/10min | ||
密度 | ASTM D-1505 | 0.921 | g/cc | |||
機械性能 | 下降沖擊強度 | ASTM D-1709 | 130 | g | ||
拉伸抗熱強度 | MD | ASTM D-1004 | 95 | kg/cm | ||
TD | ASTM D-1004 | 90 | kg/cm | |||
抗張強度(破斷點) | ASTM D-638 | 125 | kg/cm2 | |||
斷裂伸長率 | MD | ASTM D-882 | 350 | % | ||
TD | ASTM D-882 | 500 | % | |||
延伸率(破斷點) | ASTM D-638 | 700 | % | |||
斷裂拉伸強度 | MD | ASTM D-882 | 230 | kg/cm2 | ||
TD | ASTM D-882 | 200 | kg/cm2 | |||
熱性能 | 熔點 | ASTM D-2117 | 108 | ℃ | ||
維卡軟化點 | ASTM D-1525 | 90 | ℃ | |||
其它性能 | 厚度 | HCC | 0.06 | ㎜ | ||
混濁度 | ASTM D-1009 | 6.0 | % | |||
光澤度 | 45 | ASTM D-2457 | 75 | % |